Melting Points of Polymers

Polymer Name Tm1
(°C)
Poly(tetramethylene oxide), PTMO 41, 60
Poly(ethylene adipate) 63
Poly(ethylene oxide), PEG 66
Poly(trans-1,4-butadiene) 98
PoIy(1-butene), isotactic 124
Poly(ethylene) 141
Poly(methyl methacrylate), isotactic 144
Poly(trans-1,4-butadiene) 144
Poly(methylene oxide), POM 172
Poly(vinylidene fluoride) 176
Poly(propylene), isotactic 179
Poly(ω-undecanamide), Nylon 11 187
Poly(vinyl fluoride) 199
Poly(methyl methacrylate), syndiotactic 200
Poly(vinylidene chloride) 202
Poly(decamethylene sebacamide), Nylon 10,10 202
Poly(vinyl chloride) 220
Poly(caprolactam) 222
Poly(6-aminocaproic acid) 224
Poly(hexamethylene sebacamide), Nylon 6,10 224
Poly(vinyl alcohol) 231
Poly(decamethylene adipamide), Nylon 10,6 235
Poly(hexamethylene suberamide), Nylon 6,8 236
Poly(styrene), isotactic 242
Poly(4-methylpentene) 243
Poly(ethylene terephthalate), PET 264
Poly(hexamethylene adipamide), Nylon 6,6 272
Poly(styrene), syndiotactic 276
Poly(vinyl chloride), PVC 305
Poly(acrylonitrile), syndiotactic 321
Poly(etheretherketone), PEEK 357
1The Tms are the average of several experimental values.